GB/T8163 VS GB9948

2021-11-12
GB/T8163 VS GB9948The difference between GB/T8163 seamless steel pipe and GB9948 seamless steel pipe
 
GB/T8163-2008 Seamless steel pipe for conveying fluid: general seamless steel pipe for conveying fluid.
GB9948-2013 Seamless steel pipe for petroleum cracking: suitable for seamless pipes of furnace tubes, heat exchanger tubes and pipelines in petroleum refineries.

different GB/T8163 GB9948 note
Tolerance of outer diameter and wall thickness
OD>10~30
Ordinary level high-level OD≤30 ±0.20 Cold drawn (rolled) tube
±0.40 ±0.20

WT>1~3
+15% +12.5% WT≤3 +12%
-10%
-10% -10%
Steel grade and
chemical composition
Should comply with GB/T699 or GB/T1591
C:0.07~0.13%
Mn: 0.35~0.65%
C:0.17~0.23%
Mn: 0.35~0.65%
C:0.07~0.14% 
Mn: 0.35~0.65%
C:0.17~0.24%
Mn: 0.35~0.65%
High quality carbon steel:
10#
 
20#
delivery status Hot rolled tube hot rolled, cold drawn (rolled) tube in heat treated state (generally annealed)
 
Hot rolled tube finishing, cold drawn tube normalizing  
Mechanical properties 10# σb=335~475MPa
σs≥205MPa 
δ5≥24%
σb=330~490MPa
σs≥205MPa  
δ5≥24%

 
 
20# σb=410~550MPa
σs≥245MPa
δ5≥20%
σb=410~550MPa
σs≥245MPa  
δ5≥21%

 
Hydrostatictest The steel pipe shall be hydraulically tested one by one, the maximum pressure shall not exceed 19 MPa, and the withstand voltage shall be not less than 5 s, P = 2SR/D The steel pipe shall be hydraulically tested one by one, the maximum pressure shall not exceed 20 MPa, and the withstand voltage shall not be less than 10 s, P=2SR/D
 
Suppliers can use ultrasonic testing and eddy current testing instead of hydraulic test
Flattening test 22≤OD≤400 and wall thickness/outer diameter ≤10% Steel pipe with outer diameter >22~400 No cracks or cracks are allowed on the specimen after the flattening test
 
Flaring test Wall thickness ≤ 8 can be done Wall thickness ≤ 8 and outer diameter ≤ 159 No cracks or cracks shall appear on the specimen
 
Bending test Steel pipe with outer diameter ≤22 / No cracks or cracks in the bend
 
Surface Quality The inner and outer surfaces of the steel pipe shall be free from cracks, folds, rolling, separation and crusting. Other defects whose depth does not exceed the negative deviation of the wall thickness are allowed to exist.
 
The inner and outer surfaces of the steel pipe shall not have cracks, folds, rolling, separation, crusting and hairline defects. Other defects that do not exceed the negative deviation of the wall thickness are allowed to exist.
 
 
Non-destructive testing   Steel pipes should be ultrasonically tested one by one
 
 


Noteσb=Tensile Strength(MPa),  σs=Yield Strength(MPa),  δ5=Elongation(%)

 
Mail consultation